Santoprene™ 591-65W175

Santoprene™ 591-65W175

Santoprene™ 591-65W175

TPV(热塑性硫化弹性体)

埃克森美孚化工(ExxonMobil Chemical)

产品描述

Santoprene™ 591-65W175 is a soft, black thermoplastic vulcanizate (TPV) in the thermoplastic elastomer (TPE) family. This material is designed for thin wall, architectural glazing and sealing applications in industry and consumer segments. This grade of Santoprene™ TPV is shear-dependent and can be processed on conventional thermoplastics equipment for extrusion, thermoforming. It is polyolefin based and completely recyclable.


Key Features 

• Recommended for glazing and sealing applications in industry and consumer segments. 

• Excellent resistance to compression set. 

• Designed for extruding thin sections with excellent definition (down to 0.33 mm [0.013"] radius). Long runs with minimal build-up of material on screen packs or narrow sections die sections.

基本信息
原厂资料
物性表(英文)
物性表(中文)
产品特性
软质
颜色形状
粒状
黑色
成型方式
挤出
片材挤出
型材挤出
热成型
共挤
技术参数
物理性能 值/单位 测试标准 测试条件

密度

0.987 g/cm³ ASTM D792
机械性能 值/单位 测试标准 测试条件

拉伸强度

断裂(brk)

7.03 Mpa ASTM D 412
Across Flow, 23°C

100%延伸率时

2.94 Mpa ASTM D 412
Across Flow, 23°C

拉伸延伸率

断裂(brk)

440 % ASTM D 412
Across Flow, 23°C

压缩永久形变

45 % ASTM D 395
125°C, 70 hr, Type 1

压缩永久形变

31 % ASTM D 395
70°C, 22 hr, Type 1
硬度性能 值/单位 测试标准 测试条件

邵氏硬度 A

73 A ISO 868
15 sec, 23°C
老化性能 值/单位 测试标准 测试条件

硬度 (热老化)

0.3 - ASTM D573
Change in Air, 150°C, 168 hr

拉伸强度(热老化)

-6.4 % ASTM D573
Change in Air, 150°C, 168 hr

延伸率(热老化)

-4.7 % ASTM D573
Change in Air, 150°C, 168 hr